The SNAG Lifetime Achievement Award is presented each year, at the annual conference.Jurors Bernard Bernstein, Lane Coulter and Mary Ann Scherr unanimously chose Cynthia Eid's vessel as the winning design in SNAG's design competition for the award. It is an Argentium Sterling Bowl 3" X 3" X 3, on a marble base. The anticlastic rim is engraved in commemoration of the honoree.This year's recipient is Lois Betteridge. Past honorees include Stanley Lechtzin, Heikki Seppa, and Mary Ann Scherr.
Process-Part I: Deep Drawing in a Hydraulic Press

Argentium Silver sheet ready for microfolding
microfolding (corrugation) .3mm thick Argentium Sterling Silver
- Argentium sterling silver sheet was microfolded (corrugated) in a microfold brake. After annealing, it was microfolded again, at an angle to the first direction. Repeated annealing and microfolding was necessary to achieve the depth of the texture.
- The textured silver sheet was cut into a circle.
- The disc will be formed by deep drawing in a hydraulic press
The rim is formed from a seamless cylinder made by deep drawing a disc of sterling sheet in the hydraulic press, and then cutting a “slice” of the resulting cylinder. This was then formed using Bonny Doon’s anticlastic forming tools in the hydraulic press. The rim and bowl were carefully matched and fitted together. Silver brazing these two parts together was tricky—getting the alignment right, and avoiding having the solder fill the texture were exacting procedures.
The base was made in a similar manner to the rim.
Deep drawing in the hydraulic press. This is a re-draw: making the silver form taller and narrower. the steel dies form the metal. the delrin rings create space for the vessel to form into.
The hydraulic press part of the process is completed. In the foreground, are the bowl, foot, and rim. In the background they are stacked together.
PROCESS – PART II: Anticlasting, Silver Soldering, and Finishing
The rim is (conveniently!) just the right size to be formed with Bonny Doon's delrin anticlastic former in a hydraulic press. Sometimes it comes out just right, but I usually need to do a bit by hand with a mallet and anticlastic stake to get it to fit the bowl. This photo shows the tools, partially set up to use---under pressure, the urethane pushes the silver against the delrin anticlastic former.
The three forms are ready to fit and silver solder together.
Binding wire holds the foot in place. The silver around the foot is painted with "stop-off" to make sure the solder does not go where it is not wanted.
The foot was protected by carborundum grain while the rim was soldered on from the inside. Since the rim had been sanded smooth before soldering, the copper in the Argentium Sterling discolored, just like traditional sterling.
I am very careful about keeping my studio and kitchen separate, with the exception of using my kitchen oven to harden the Argentium Sterling.












{ 5 comments… read them below or add one }
Hmmm….Life is curious. Here I am, in 2012, making this year’s award, and checking my blog to remind myself what my process is!
C Eid
What an amazing and inspiring process post!
Thank you!!!
Cynthia,
Congratulations on the Lifetime Achievement Award. It is well deserved! Also, thanks for sharing the process with us for the bowl. It is a beautiful bowl, and process isn’t immediately evident for those of us who are inexperienced in drawing. Again, Congrats!
Jamie
Thank you for sharing this. What a gorgeous, timeless piece.
I have always admired this piece. Even though I knew how you created it, your clear, concise information set cleared up a couple of questions.
Thank you for making this available.
Lee (the saw guy)