earrings, gold and brilliantsThe earrings,  polished just too much, lost some crispness


Made two tubes of the right diameter (the crown of the stone rests in the thickness of thetube), made four holes in the circumference at middle height.


enlarging the holes, will leave between them the thickness of a prong

cut in half the tube

to get two pronged bezels

some filing with the round file to set the inclination and regularize the prongs

here are the four (I’ making two pair of earrings) bezels, the prongs are ok

a nick with the saw just under the prongs

with a square file the nick is enlarged and deepened, the bezel is held in a piece of wood

ready for the back

the paillons are in place

the bottom has been soldered and cut in circle

to solder the stem, I heat the bottom of the bezel on which a paillon is placed, and keep the stem near the flame. When the paillon starts melting I rest the stem on it, wait till the solder wets bezel and stem, take away the flame and wait for the solder to set before opening the tweezers.

I nick the inside of each prong with the saw, a little filing with a triangular file will perfect the notch.

 

the stone enters with a click


some beading over the tip of the prongs

forgot to say that I made a groove at the bottom of the bezels

The butterfly nuts are 0.6 mm thick, somewhere between gauge 24 and 22.  First I cut the shape, with a round punch I deepen the center and bore a hole. With a tracer punch I  make a groove in the middle of the wings

Then I  roll up the wings until they will let the stem pass through with a little effort.  Just a little under the end of the stem I made a circular groove with round nosed pliers: the butterfly nut clicks in the groove and stays secure.

I JUST SAW THAT I’VE USED UP 94% OF THE SPACE GANOKSIN ALLOWS ME TO USE.
ANY SUGGESTION ON HOW TO GO ON?
I was planning to post an article on the unconventional use of the wire rolling mills.
Goodbye, Mario

 

{ 7 comments }

a rather heavy ballpoint pen


 

Describing a rather detailed step by step construction of a ballpoint pen in silver.
The signature of the recipient of this gift and the carving of the eagle have been covered with pure gold with the kum-boo technique. Threadings and other small parts are of brass.
You will see some problems I met and how I solved them. You will see a catastrophic event take place.

A friend of mine told me that I should have cleaned my nails before taking this photo.


This is the cross section of the final pen, the yellow parts are of brass.
It shows only the main parts, but often I had to add a small piece here and there either for functional or aestethical reasons, or to reach the needed fitting size.
The lid is screwed to the body to close the pen,  it  can be screwed to  the other end of the body.
The clip is tightened screwing the brass dome into the top of the lid (top, outside).
The grip is hourglass shaped; the point of the refill is blocked by a small brass ring at the end of the cone tat ends the pen (top, inside).
The refill is pushed towards the point of the pen by a steel spring (bottom, inside), one end of it holds a sphere of silver soldered to a small tube into which the refill enters; the other end of the spring rests inside the brass dome that is screwed into the end of the pen (bottom, outside).

 


 

 

Found the right diameter for the body (the client wanted a heavy pen) I cut the sheet and rolled it.

 

 


The tube after soldering and straightening.

 


I cut the female thread from a burner and the male thread from a camping gaz connector. The male thread needed to be lenghtened to enter into the body of the pen so I soldered to it a piece of copper tube.

 

I carved a seat at the end of the thread (left) to accomodate the small silver cone (center) on which the longer hourglass shaped tube (right) will be soldered. Had to do it for fitting reasons, the circumference of the rim left on the brass thread is too small for the base of the hourglass.

Ready for soldering


 

The silver cone that will make the point of the pen, just soldered.

The cone cleaned, filed a bit and brought to measure, I beveled the inside of the hourglass and the outside of the cone to get an horizontal good fit. The copper back of the brass thread is just resting inside the body, not yet soldered to it.

Ready for soldering, the binding wire is inside, tightened between a cotter pin on the large hole and another cotter pin resting on a kind of thick washer overlapping  the smaller hole, not to damage it.


Filed the brass thread that enters the lid

The female brass thread has been soldered to the lid, and screwed to the male brass thread which has also been soldered to the body of the pen.
A small dome is just inserted on the free end of the lid, the other dome is waiting to be used.

Preparing the cap of the body: the external thread on the brass tube (left) had to be completely hand made with saw and file. The tube is threaded inside, on the right you can see the threaded cylinder which will be screwed inside the tube.

In the middle you see the dome that will be soldered to the threaded cylinder.

The dome is soldered


I file the brass dome that will be the cap of the lid, rounding it, and drill a hole on its side where a piece of thick wire will be soldered. This wire will be hammered in the shape of the clip, therefore hardened, after the unavoidable annealing due to the soldering.
This is the first version of the clip, not the the final one.

Back to the cap of the body: dissatisfied with the first hand made thread, decided to turn the tube over and make a new one. The tube does not fill the inside of the body, so to keep it in the center I raised a few small prongs all around its surface with a graver.

 The tube has been soldered to the top of the body, with the graver I have carved four areas near the point, they will make pendant with the ones I just draw on the lid.

The threaded cylinder is wound turning the dome to which it is soldered.

I prepared a coil spring with piano wire, resting inside the threaded cylinder, the spring works on the bottom of a silver short tube that grabs the refill.

You can see the shape of the forged clip, the basic decoration: the areas are rendered matt and blackened with liver of sulphur.


Now the structure is over, must think about the eagle and the signature. Found the right eagle, painted white the silver surface, taped the double faced drawing and transferred the drawing. Done the same with signature.

It is a delicate moment, carving allows for no mistakes, so I first tried on an aluminum tube.

The beginning strokes of the graver on the silver.

Carving the feathers.

 The carving of the eagle is done, must always remember to reach the right amount of detail, but no more than is needed.            “Surtout, pas trop de zèle.”

 

The kum-boo technique asks you to enrich the surface of the alloyed silver. You must anneal the silver, let it cool and plunge in sulphuric acid to remove the copper that oxidizes. Doing it four or five times brings the surface to pure silver state.
In the above image you see that only the eagle (and the carved signature) shows the brown colors of oxidised copper; this is because carving has exposed new layers not yet freed of surface copper while the rest of the surface of the pen has been annealed and acid cleaned because of the solderings and is almost free of oxides.


I annealed and immersed in acid the pen a few times, after the last annealing I forgot the pen in the acid and had the opportunity to learn from experience that prolonged immersion in sulphuric acid eats away brass.

 

 

This is what I found the morning after.

 

 

 

 

 


 So.. let us start again!

Must do things with precision, to keep everything in axis.

Fitting the brass thread in the middle of the pen.

Preparing the clip, the female thread having alreadybeen  soldered to the top of the lid, the male one is waiting to be topped with a brass dome.

All the pieces waiting for assembly.

The pen with the gold foil to be used for kum boo.


The batteries of my camera were finished, so I could not take photographs of the kum boo application of the gold foil: everything was working well and I did not want to wait and lose concentration.  Anyhow this is the result, finished and polished.

In its velvet lined wooden handmade case.

Mi piaceVisualizzazioni: 58

 

{ 7 comments }

cages necklace

by Mario Cesari on October 23, 2011 · 9 comments

in Uncategorized

A simple necklace, made of iron wire

you just need a mandrel, snippers, round nose and flat nose pliers

make a coil around the mandrel (can be iron, wood or any material), don’t need to be precise

 

cut a series of almost 2 coils (or one and three quarter coil)

 

with round nose pliers make a loop at both extremities

 

with flat nose pliers bend the coil twice at half circle lenght

 

now let them enter into each other the way you see in the picture

 

close the loop so that it grasps the bend

 

when you’ve added enough pieces, add a ring and a hook for closure

 

instead of interlocking the pieces, if the end loop is wide enough, you can connect each piece with a small ring.

 

 

 

{ 9 comments }

You can make swords from nails for your chipmunks, sure, but what about
defensive measures? You must provide your chipmunks with shields.
Here’ a short tutorial on how to make a shield from a tuna can lid.

me holding a chipmunk shieldThis is the finished shield, chipmunk-size.

Here’s a tuna can lid, the right size, I had complaints when using soup can lids: too heavy.
I put it in the fire (my woodstove is already going, rather cold here in the mountains) to soften it and to burn away paint, coating etc. The tab comes away easily without pliers or any tool, just bend it the other way once or twice and it will break free.

It is a good practice to carve a few cavities of different depth in a log, each about the same width. Lean the disk over one of the cavities, preferably a shallow one,  and start hammering near the rim all around the circumference.

Go on hammering in concentic circles towards the center. If crimples arise, level them starting from where they begin.

For planishing you must find a round headed stake, it can be a hammer in a vise, of suitable curve.

Then with the flat face of the hammer go over the whole surface of the shallow bowl.

With a nail punch a hole near the rim.

 

Do the same on the opposite side, enlarge the holes to let a piece of iron wire pass through them. Bend the wire and insert it.

 

Bend the ends of the wire over the rim,

 

cut the excess,

 

and squeeze the ends of the wire against the rim.

 

sword and shield kitSword and shield.

You can have this S&S kit for only 499 nuts.

 

 

 

{ 5 comments }

Forging is fun. Steel needs to be hot forged but iron can be cold forged, needing only to be annealed when hammering has hardened it.

nails

three small knives

Common nails are made of iron. Sometimes common nails can be  of mild steel, in which case you must anneal them (bringing the steel to red-heath and letting it air-cool) when you notice they are hardening.  Any nail, around 3 inches long, can be turned into a small knife, old bent nails cost nothing so you can try and explore different shapes at no cost and in no time.
Or you can make small traditional shapes such as scimitar, kukri, kriss (haven’t tried yet).

To make a simple blade

bending a nail 1) The blade has to be thinner on the cutting edge and thicker on the back, but the edge that gets thinner becomes longer because the squeezed metal must find space anyway: your blade would bend upwards.
So you first slightly bend the blade then hammer the inside of the curve.

2) Blow after blow you will see the blade straightening. The point of the nail gets the right shape by itself if you hammer it evenly.

3) The stake you’re hammering on had better be a bit rounded since you have to “pinch” more one side of the blade.

4) Now you can round off the head of the nail, hammering its edge. As the diameter of the head diminishes, a protruding edge develops on both sides of the head.

 

5) You tuck in this edge.

6) You flatten the part of the nail between the head and the blade to make the shank.

7) Now you must anneal the shank: bring it to red heath with a flame and leti it air cool.

8) Hold the shank with two pliers and twist it.

9) Some hammer blows on the twist will straighten it. Now you have a small handle with a good grip.

10) Hammer work is over, notice the colour changes from black where the iron was heated, to blue and yellow.

Now you can file the blade to sharpen it and do a bit of filing on  the shank.

11) If you want you can hone the cutting edge and go over the rest of the knife with different grades of abrasive paper. Don’t overdo it, a kind of roughness is part of blacksmithing’s appeal.

{ 13 comments }

Mario Cesari
Born in Venezia, Italy, metalworker for thirty-odd years, learning blacksmithing and chasing in London, cuttlefish bone casting and jewel construction back in Venezia, small-scale sand casting and other traditional nepalese techniques in Katmandu.
Went to live in the country and learnt forge welding and Damascus steel making, attended seminar on Ancient Etruscan Techniques and learnt granulation, made replicas of scientific instruments for museums. In 1999 at UGA in Athens, GA, as visiting artist.
Translated Metalwork and enameling by H. Maryon, wrote articles for Italian and American crafts magazines.
In the last years mostly researching, teaching and taking care of my site http://www.pennabilli.org